For most external structural steelwork and architectural metalwork in the UK, the choice comes down to hot-dip galvanising, a paint system, or a combination of both applied as a duplex system. Each has a different maintenance cycle, appearance, and suitability for specific environments. The right decision depends on the exposure category, the required service life, the dimensions of the components, and whether the steelwork will be accessible for repainting once it is in place.

Hot-dip galvanising and BS EN ISO 1461

Hot-dip galvanising dips fabricated steel into molten zinc at around 450°C. The zinc reacts with the steel surface to form a metallurgical bond, not merely a surface layer. The result is harder than zinc alone and provides cathodic (sacrificial) protection: where the coating is damaged, the zinc around the exposed area continues to protect the underlying steel.

The current British and European specification for this process is BS EN ISO 1461:2022, which replaced the older BS 729. The standard sets minimum zinc coating thicknesses based on the thickness of the steel being coated. For structural sections where the steel is more than 6 mm thick, the required mean minimum coating is 85 μm. According to steelconstruction.info, abrasive blast-cleaned steel and thicker sections draw more zinc from the bath, so actual coatings on structural work regularly reach around 140 μm, well above the minimum. The Galvanizers Association notes that a galvanised coating can last over 100 years, and that lifespan estimates based on minimum thickness are conservative because actual coatings typically exceed the standard minimum.

Design matters here too. Hollow sections need vent, fill, and drain holes to allow molten zinc to flow through and back out; closed cavities cannot be galvanised safely. For structural work that will be galvanised, specifying an Option 5 steel to BS EN 10025-1 ensures the steel chemistry is suitable for the process, as steelconstruction.info notes.

Size constraints

Steelwork must physically fit into the galvanising bath, and every plant has different bath dimensions. According to steelconstruction.info, the longest galvanising tank currently operating in the UK is 21 m, with a maximum double-dip capacity of 28 m and a maximum lift weight of 16 tonnes. Double-dipping involves immersing one end of a longer piece, withdrawing it, and dipping the other end; the corrosion protection from double-dipping is identical to a single dip.

For staircases, balustrades, gates, and the structural beams and columns typical of commercial and residential work, bath size is rarely a constraint. For large structural frames with long or heavy members, it is worth confirming with a galvanising plant early in the design process. Dimensions and weight can affect what is feasible and may influence the erection sequence or connection detailing.

Paint systems and BS EN ISO 12944

Paint system selection for external steelwork uses BS EN ISO 12944. Part 2 of the standard classifies atmospheric corrosivity from C1 (very low: clean heated interiors) to C5 (very high: high-salinity coastal or high-humidity industrial environments), with CX for offshore structures. Part 5 lists paint systems suited to each category and gives a coating life, defined as the expected time before first major maintenance. Coating life is a maintenance planning figure, not a performance guarantee.

The category that applies depends on location and local conditions. East Sussex includes inland rural and urban areas, which typically fall into C2 or C3, and coastal locations where C4 may apply. Distance from the sea, prevailing wind direction, and local industrial activity all affect the result. A structural balustrade close to the coast sits in a significantly more aggressive environment than one in an inland garden.

CategoryTypical environmentExample systemCoating life
C3Urban or industrial, moderate pollution; low-salinity coastalHot-dip galvanised (≥85 μm, steel >6 mm)20+ years
C3As aboveBlast Sa 2½; zinc phosphate epoxy primer 80 μm + epoxy MIO 100 μm + PU finish 60 μm20 years
C4Industrial or moderate-salinity coastalBlast Sa 2½; zinc-rich epoxy primer 40 μm + epoxy MIO 100 μm; site epoxy MIO 100 μm15–20 years
C5High-humidity industrial or high-salinity coastalBlast Sa 2½; zinc-rich epoxy primer 40 μm + epoxy MIO 200 μm; site aliphatic PU 60 μm20 years

Source: steelconstruction.info standard corrosion protection systems for buildings, based on BS EN ISO 12944.

Duplex systems

A duplex system applies a paint topcoat over hot-dip galvanising. The two coatings work in different ways: the paint acts as a barrier that slows the rate at which the zinc is consumed, and the zinc continues to provide sacrificial protection if the paint layer is breached. Steelconstruction.info describes the combination as more durable than either coating alone.

Surface preparation before painting is critical and is the most common source of adhesion failure on galvanised steel. According to steelconstruction.info, galvanised surfaces must be treated with a mordant wash (also known as T-wash, an acidified solution that provides a visual check of coverage), an etch primer, or sweep blasting before the paint system is applied. Applying a paint system formulated for bare steel directly to galvanised steel without this preparation typically results in adhesion failure.

One standard duplex system at BS EN ISO 12944 C5 level, as listed in steelconstruction.info’s standard systems table, uses hot-dip galvanising (≥85 μm), followed by mordant wash, etch primer, factory-applied epoxy MIO primer, and a site-applied polyurethane finish, giving a 15-year coating life. Higher initial cost may be justified for steelwork in aggressive environments where access for repainting would be difficult or disruptive.

Welds and site cuts

Galvanising takes place after fabrication is complete. Any welding, cutting, or drilling carried out on site after delivery breaks the zinc coating at those points. Site connections on structural steelwork and on-site fitting adjustments are common situations where this occurs.

BS EN ISO 1461 permits repair of uncoated areas up to 10 cm² each. The Galvanizers Association confirms three accepted repair methods: zinc-rich paint or paste, a low-melting-point zinc stick, or zinc thermal spraying, with a minimum repair thickness of 100 μm unless otherwise agreed. Total repairs must not exceed 0.5% of the article’s surface area. Larger uncoated areas require regalvanising unless otherwise agreed with the galvaniser.

For paint-only systems, site welds and cuts must be ground back to clean metal and reprimed to the paint system specification before the topcoat is applied. The surface preparation grade and repriming coat depend on the system specified.

Cost and maintenance

Specific costs depend on section sizes, finish complexity, transport to the galvanising plant, and current market rates. No meaningful comparison figures are given here. Qualitatively:

  • Galvanising suits external work with a long required service life and limited maintenance access, because the coating requires little ongoing attention once applied
  • Paint systems offer more colour choice and are not constrained by bath dimensions, but require periodic inspection and repainting when the coating life is reached
  • Duplex systems carry higher initial cost but can reduce whole-life cost for exposed or coastal locations where future repainting would be expensive or impractical

For projects in C4 or C5 environments, the appropriate finish specification should be confirmed by a structural engineer or corrosion specialist.

For guidance on finishes for a specific project, get in touch via twojsmetalwork.co.uk/contact-metal-fabricators.

Share

Written by Two Js Metalwork

Structural steel fabrication and architectural metalwork in Sussex. See the projects behind the advice.

Start Your Project

Get in touch to discuss your steel fabrication requirements.

Call Two Js Metalwork